Ti-6Al-4V

Wrought As-Cast (Annealed)

EBM As- Deposited

EBM HIP'ed

Ultimate Tensile Strength, Mpa

1000

930

1037 +/- 28

957 +/- 13

Yield Strength, Mpa

896

885

948 +/- 27

905 +/- 19

20

RT Tensile Properties for EBM Titanium-6Al-4V

44.4 +/- 9

57.5 +/- 5

15.5 +/- 1.9

17.2 +/- 1.5

Strength, ksi

145 135

150 +/- 4

139 +/- 2

Yield Strength, ksi

130 128

137 +/- 4

131 +/- 3

12

Reduction of Area, %